Silane Tanned Leather and
Administrative Litigation
love brother love sister
love righteousness
A silane tanning process of replacing enzyme preparation with water-soluble polyamine silane coupling agent
- Categories:发明专利
- Author:
- Origin:
- Time of issue:2020-01-10 11:01
- Views:
(Summary description)The invention relates to a silane tanning process of replacing enzyme preparation with water-soluble polyamine silane coupling agent, which has the advantages of simple and stable operation mode and easy to understand process. Save more than 50% of time and more than 40% of water, significantly reduce the emission of pollutants and the consumption of water, electricity, manpower and other resources.
A silane tanning process of replacing enzyme preparation with water-soluble polyamine silane coupling agent
(Summary description)The invention relates to a silane tanning process of replacing enzyme preparation with water-soluble polyamine silane coupling agent, which has the advantages of simple and stable operation mode and easy to understand process. Save more than 50% of time and more than 40% of water, significantly reduce the emission of pollutants and the consumption of water, electricity, manpower and other resources.
- Categories:发明专利
- Author:
- Origin:
- Time of issue:2020-01-10 11:01
- Views:
right-claiming document
1. A silane tanning process using water-soluble polyamine silane coupling agent instead of enzyme preparation, including fur silane soaking, silica gel ash coating and wool pushing, silane alkali sulfide wool destroying and liming, silica gel re liming, silane hydrogen peroxide pre Liming (eliminating alkali sulfide), silane hydrogen peroxide main Liming (eliminating alkali sulfide), cationic silica gel pretreatment, salt leaching, acid leaching Silicone aldehyde primary tanning / silica gel tannin extract combined primary tanning, cationic silica gel softening, anionic silica gel tannin extract dyeing, retanning, filling and fatliquoring, cationic silica gel fixation and mildew proof treatment, which are characterized by:
(1) The silane soaking step of the fur is as follows: weigh 100 parts of fur by weight in the drum, wash with water for 10 minutes, add 100-150 parts of normal temperature water, 0.1-1 parts of kt1717, 0.05-0.3 parts of kt3007, 0.2-0.5 parts of non-ionic degreasing agent, 0.1-0.3 parts of bactericide, 0.3-1 parts of soda ash and 0.1-0.3 parts of sodium sulfide, rotate slowly for 3 hours, rotate for 30 minutes / stop for 30 minutes, and rotate for 8-10 hours, In this step, no soaking enzyme or degreasing enzyme is needed, the drum is out, the meat is removed, and the ash is wrapped in silica gel to push the hair;
(2) The silica gel ash coating and roughening steps are as follows: 5000 parts of water, 30-60 parts of kt1717, 15-40 parts of kt3007, 20-40 parts of Liming additives, 30-60 parts of non-ionic degreasing agent, 60-100 parts of sodium hydrosulfide and 240-280 parts of sodium sulfide by weight; Mix well, then slowly add 3000-4000 parts of lime, mix while adding, and mix well to obtain mortar; Coat the coated mortar on the fur meat surface, increase the amount of ridge line application appropriately, overlap the meat, and stand for 6-24 hours. In this step, do not use Liming enzyme and other alkaline enzymes, push the wool, and enter silane alkali sulfide to destroy the wool and liming;
(3) The silane alkali sulfide wool destroying and liming steps are as follows: add 10-30 parts of normal temperature water, 0.1-0.3 parts of kt1717, 0.3-0.5 parts of non-ionic degreasing agent, 0.3-0.5 parts of Liming assistant, 0.5-0.8 parts of sodium hydrosulfide and 0.5-0.8 parts of sodium sulfide, turn for 30 minutes / stop for 30 minutes and 2 hours after slow rotation for 1 hour; Add 0.5-1 part of kt1717, 0.5-1.5 part of alkali sulfide and 1-3 part of lime, turn for 30 minutes / stop for 30 minutes and turn for 2 hours; Add 0.5-1 part of kt1717, 0.5-1.5 part of alkali sulfide and 1-3 part of lime, turn for 30 minutes / stop for 30 minutes and turn for 2-12 hours; Check the wool destruction. After the wool is destroyed, add 1-5 parts of kt1717, rotate for 2 hours, add 30-50 parts of normal temperature water, 1-2 parts of lime and 0.1-0.3 parts of Liming Agent, rotate for 30 minutes / stop for 30 minutes and stop for 2 hours; Add 50-150 phr of normal temperature water, 1-2 phr of lime and 0.1-0.3 phr of Liming aid, turn for 30 minutes / stop for 30 minutes, turn for 5 minutes / stop for 55 minutes after 2 hours, and turn for 10-24 hours. In this step, the drum skin is produced without Liming enzyme and other alkaline enzymes. The waste liquid is retained and can be recycled as Liming solution or re Liming solution, and then enter silica gel for re Liming;
(4) The silica gel re ashing steps are as follows: weigh 100 parts of alkali skin into the drum by weight, add 100-200 parts of wool destroying Liming waste liquid, add 1-2 parts of kt1717, 0.3-0.5 parts of non-ionic degreasing agent and 3-5 parts of lime, turn slowly for 30 minutes / stop for 30 minutes and stop for 4-12 hours. Liming enzyme and other alkaline enzymes are not used in this step; The waste liquid can be used as Liming solution or re Liming solution for recycling. Wash the ash skin with water and enter silane hydrogen peroxide for pre deashing (eliminate alkali sulfide);
(5) The silane hydrogen peroxide pre deashing (eliminating alkali sulfide) step is as follows: add 50-100 parts of normal temperature water, 1-2 parts of kt1717, 0.3-0.5 parts of non-ionic degreasing agent, and rotate slowly for 2 hours; Add 3-5 parts of ammonium sulfate and 0.5-1 part of deashing agent, and rotate slowly for 2 hours; Add 1-2 parts of hydrogen peroxide and rotate slowly for 4 hours. In this step, do not use softening enzymes such as trypsin and 1398 alkaline enzyme, wash with water, and enter silane hydrogen peroxide for main deashing (eliminate alkali sulfide);
(6) The main deashing (eliminating alkali sulfide) step of silane hydrogen peroxide is as follows: add 30-50 parts of normal temperature water, 2-4 parts of kt1717, 0.3-0.5 parts of non-ionic degreasing agent, and rotate slowly for 2 hours; Add 5-8 parts of ammonium sulfate and 0.5-1 part of deashing agent, and rotate slowly for 2 hours; Add 1-2 parts of hydrogen peroxide, rotate slowly for 4 hours, rotate slowly for 30 minutes / stop for 30 minutes, and stop for 4-12 hours; In this step, softening enzymes such as pancreatin and 1398 alkaline enzyme are not used. After washing to pH value of 6.5-7.5, softening enzymes such as pancreatin and 1398 alkaline enzyme are not used, and enter cationic silica gel for pretreatment;
(7) The pretreatment steps of cationic silica gel are as follows: add 30-50 parts of 35 ℃ hot water, 3-5 parts of kt1717 and 3-5 parts of kt4031, rotate slowly for 3 hours, and enter salt leaching;
(8) The salt leaching step is as follows: add 8-10 parts of industrial salt and 8-10 parts of sodium sulfate, rotate slowly at 35 ℃ for 3 hours, and enter acid leaching;
(9) The acid leaching step is as follows: add 0.5-1.5 phr of industrial formic acid, adjust the pH value range to 2.5-3, rotate slowly for 8-12 hours, and enter silicone aldehyde primary tanning / silica gel tannin extract combined primary tanning;
(10) The initial tanning steps of silicone aldehyde / silica gel tannin extract combination are as follows: adding 3-5 parts of kt2811, 0.1-0.3 parts of acid resistant oil and 2-4 parts of kt2034, and rotating slowly for 4-8 hours; Add 8-16 parts of tannin extract, 2-4 parts of acid resistant oil, 4-6 parts of kt2034 and 2-4 parts of kt5901, and rotate slowly for 8-12 hours; Add 1-2 parts of acid resistant oil and 2-4 parts of kt2034, adjust the temperature to 45 ℃, and rotate slowly for 8-12 hours; Leave the drum to stand for 48 hours, squeeze and cut evenly, and enter the cationic silica gel to soften;
(11) The softening step of the cationic silica gel is as follows: weigh 100 parts of the peeled primary tanning skin according to the weight, put it in the drum, wash it twice, and adjust the temperature to 45 ℃; Add 100-150 parts of water at 45 ℃, kt4031 5-8 parts, kt1717 5-8 parts and kt2811 1-3 parts, rotate at medium speed for 4-6 hours, add 1-2 parts of baking soda and rotate at medium speed for 4-6 hours. This step does not need acid enzyme treatment, enter anionic silica gel tannin extract dyeing retanning, filling and fatliquoring;
(12) The anionic silica gel tannin extract dyeing, retanning, filling and fatliquoring steps are as follows: adding x parts of dye, 3-5 parts of tannin extract, 2-4 parts of kt5901, 6-8 parts of kt2034, 4-6 parts of kt2351, 3-5 parts of acid resistant oil and 5-8 parts of general oil in the same bath, rotating at a medium speed of 45 ℃ for 8-12 hours, and entering cationic silica gel fixation and anti mildew treatment;
(13) The cationic silica gel fixing and anti mildew treatment steps are: adding formic acid in the same bath to adjust the pH value to 3-3.5, rotating at a medium speed of 45 ℃ for 1 hour, adding 1-3 parts of kt4031 and 0.3-0.5 parts of anti mildew agent, rotating at a medium speed of 45 ℃ for 2 hours, washing twice, bulging, drying and finishing to obtain leather blank.
2. the water-saving and emission reducing silane tanning process is completely replaced by water soluble polymer polyamine silane coupling agent according to claim 1. The characteristics are as follows: the KT1717 is a soft replacement and silane, and KT1717 is a side polyalkyl polyhydroxyalkyl triethoxy silyl based polymethylsilsesquioxane water emulsion with weak cationic emulsion polymerization. Also known as: water soluble silicone high molecular silane coupling agent, low temperature coupling self crosslinking aminoalkyl hydroxyalkyl silicone oil. The technical indexes are: 20 ℃ density 0.95 g / ml, water-soluble content 20 ± 1%, solvent water, pH value 6.5 ± 0.2, viscosity 40-50 MPa S, the appearance is light blue emulsion.
3. The water-saving and emission reducing silane tanning process of completely replacing biological enzyme preparation with water-soluble polymer polyamine silane coupling agent according to claim 1, which is characterized in that kt3007 is an osmotic crosslinking silane assistant, kt3007 is an aqueous solution of poly epoxy alcohol ether alkyl polymethylsiloxane silane coupling agent isopropanol, and the technical index is: 20 ℃ density 0.85g/ml, Weight percentage of nonvolatile component: 36 ± 1%, solvent water, pH value: 6.5 ± 0.2, charge: non-ionic, viscosity: 90-110mpa s. The appearance is light yellow to colorless transparent liquid.
4. The water-saving and emission reducing silane tanning process of completely replacing biological enzyme preparation with water-soluble polymer polyamine silane coupling agent according to claim 1, which is characterized in that kt4031 is cationic polyurethane retanning silica gel, kt4031 is a water-soluble cationic polyurethane polymer silane coupling agent with coupling cross-linking reaction activity, It is also a strong cationic polyalkoxysiloxane carbamate oil silica gel polymer; The technical indexes are: 20 ℃ density 0.95 g / ml-1.05 g / ml, water soluble content 18-22%, solvent water, pH value 4.5 ± 0.3, viscosity 400-500 MPa s. The appearance is milky yellow emulsion.
5. The water-saving and emission reducing silane tanning process of completely replacing biological enzyme preparation with water-soluble polymer polyamine silane coupling agent according to claim 1, which is characterized in that kt2811 is aminosilane modified fatty aldehyde; Kt2811 is a water-soluble silicone polyethylene polyamine polymer silane coupling agent containing aldehyde group, which has good crosslinking, hybrid modification, penetration and dispersion; The technical specifications are: pH 2-4, weak cationic charge and appearance of light blue emulsion.
6. The water-saving and emission reducing silane tanning process of completely replacing biological enzyme preparation with water-soluble high molecular polyamine silane coupling agent according to claim 1, which is characterized in that kt2034 is cotton foam fleshy filled silica gel, kt2034 is a secondary derivative of lecithin and hydroxyalkyl aminoalkyl carboxyalkyl polyalkoxysilicone modified polymethylsiloxane, and the technical index is: 20 ℃ density 0.92 g / ml, The content of water-soluble matter is 26-30%, solvent water, pH value is 3.8 ± 0.2, viscosity is 150-180mpa s. The appearance is light milky yellow thick liquid.
7. The water-soluble high molecular polyamine silane coupling agent completely replaces the water-saving and emission reduction silane tanning process of biological enzyme preparation according to claim 1, which is characterized in that kt5901 is a silicone sulfone filled synthetic tanning agent, kt5901 is a silicone sulfone bridged structure high-quality filling performance naphthol sulfonic acid and SO2 organic derivative secondary hydrolysis and condensation polymer tanning agent, Technical indicators: 20 ℃, density: 1.10g/ml-1.25 g / ml, water soluble content: 46% - 50%, solvent water, pH value: 4.0 ± 0.2, viscosity: 120MPa · s-140mpa · s, appearance: light brown, translucent and thick liquid.
8. The water-saving and emission reducing silane tanning process of completely replacing biological enzyme preparation with water-soluble polymer polyamine silane coupling agent according to claim 1, which is characterized in that kt2351 is foamed elastic fatliquoring silicone oil, kt2351 is modified polymeric silicone oil, and the modified reactive silicone oil is a water emulsion copolymer with vinyl amino and carboxyl monomers, The technical indexes are: 20 ℃ density 1.10 g / ml-1.25 g / ml, water soluble content 28-33%, solvent water, pH value 4.5-5.5, viscosity 24000-26000 MPa s. The appearance is milky yellow thick liquid.
9. The water-saving and emission reducing silane tanning process of completely replacing biological enzyme preparation with water-soluble polymer polyamine silane coupling agent according to claim 1, which is characterized in that industrial products such as kt1717, kt3007, kt2811, kt4031, kt2034, kt5901 and kt2351 are purchased from Minda silicon fluoroleather application research and test factory in Wenjiang District, Chengdu.
instructions
technical field
The invention relates to the leather field, in particular to a silane tanning process in which a water-soluble polyamine silane coupling agent replaces an enzyme preparation.
Background technology
1. Traditional vegetable tanning is the earliest method used in leather manufacturing by human beings. It uses tannin extract extracted from plants (the main component is tannin) to tannin leather. Vegetable tanned leather is the only eco-friendly leather in tanned leather. Even if it burns, it will not release toxic substances. Now some pet food is made of this kind of leather scrap. This kind of leather is thick, hard and tough. It is easy to absorb liquid. After absorbing water, it is convenient for three-dimensional plasticity. The color is light brown yellow of tannin extract; After use, the vegetable tanning leather will become dark brown after oxidation, sunshine and liquid absorption. Traditional vegetable tanned leather is mostly used for military products, mechanical accessories, basketball, belt, sole, suitcase and carved leather plastic, so it is called "heavy leather"; Because of its bitter tannin taste, it is also commonly known as "astringent skin", "tree extract skin", "tannin extract skin", etc.
2. The invention selects a water-soluble polymer silane coupling agent, that is, the water-soluble organic polymer bridged polysilsesquioxane precursor is implanted into tanning leather in the process of forming organic silica gel under alkaline conditions, which is like breast enhancement and plastic surgery. The organic silica gel is implanted into women's breasts to obtain a plump, soft and delicate meat feeling, which can completely change people's cognition of the hard and poor hand feeling of the traditional vegetable tanning board, It can obtain a brand-new silicone tannin extract combined with tanning flexible vegetable tanning leather that feels plump, soft, compact and not loose, and the leather property reaches or even exceeds that of light leather such as chrome tanned leather. This kind of leather can be in close contact with human skin, which is not only skin friendly and comfortable, but also does no harm to the skin. It can not only be used as a mat, but also make close fitting bras, underwear, etc, It will bring revolutionary innovation and subversion to the traditional leather industry, and has immeasurable environmental protection and commercial value.
3. Water soluble polymer silane coupling agent
3.1 silane coupling agent
Silane coupling agent contains both organic carbon functional group and inorganic silicon functional group, which can form a molecular bridge between inorganic and organic interface, so as to play the role of chemical tackifying, reinforcing, compatibilizing and improving the properties of composites. Silane coupling agent can be represented by [Q-R '- Si (R) NX (3-N)]. X is a hydrolyzable condensed silicon functional group, q is an organic functional group (carbon functional group), R is a Sui hydrocarbon group bonded by silicon carbon, and R' is an inert connecting group bonding silicon functional Group x and carbon functional group Q.
At present, the main products in the silane coupling agent market have small molecular weight and are mostly oil-soluble, which can not be evenly dispersed and stable in water. Before use, a large amount of alcohol is required to inhibit hydrolysis and ripen into macromolecules under acidic conditions. This process is easily affected by various conditions such as ambient temperature, humidity, medium pH and metal impurities. Its application is empirical and difficult to control, so it has certain limitations. The multifunctional polymer silane coupling agent does not need to be hydrolyzed and matured before use, but it is basically oil-soluble, not environmental friendly, and can not directly use water as the reaction medium. With the continuous development of the technology of preparing functional hybrid materials by sol-gel method in recent years, higher requirements for silane coupling agent's reactivity, controllability, repeatability, operation convenience and environmental protection have been put forward. Therefore, it is necessary to make high molecular weight, high molecular weight and water-soluble small molecule silane coupling agents.
3.2 from oil soluble and small molecules to water-soluble and high polymers
The polymerization, multi-functional and hydration of oil-soluble small molecule silane coupling agents are realized by directly connecting hydrophilic groups, multiple specific silicon functional groups, carbon functional groups and polymer bridging groups similar to the substrate structure with polysiloxane chains through hydrosilylation and acidic silane equilibrium reaction.
There are four ways to polymerize small molecule silane coupling agents: (1) grafting polyalkoxy silicon group onto organic carbon polymer chain; (2) Grafting the polysiloxane group onto the silicone polymer chain; (3) The polysiloxane group was grafted onto the polymer block copolymer chain of silicone and organic carbon; (4) The macromolecular or macromolecular silane coupling agent obtained from the above three kinds is then reactive modified with small molecular silane coupling agent or modified macromolecular silane coupling agent. The molecular weight obtained is generally greater than 10000, or even more than 30000.
In the above process, a plurality of different silicon functional groups can be introduced to realize high polymer and multi functionalization at the same time. Starting from D4 / DMC, small molecule silane coupling agent, hydrogen containing silicone oil, carbon organic monomer containing active functional group and other monomers, the small molecule silane coupling agent is polymerized into silicon organic polymer by means of hydrosilylation, copolymerization / polycondensation / grafting according to the application performance of the final product Polymer silane coupling agents containing two kinds of functional groups can be obtained by carbon organic polymerization, silicon carbon organic hybrid polymerization and further functional group modification.
Because both silicon functional groups and carbon functional groups have reaction activity, they will react in contact with active hydrogen in water. Therefore, in order to obtain silane coupling agents that can be evenly dispersed and stably exist in water, these active functional groups must be properly protected so that they will not cross-linked or inactivated by hydroxylation with water before reaching the substrate surface. The hydration of small molecule silane coupling agent starts from hydrophilic prepolymerization of monomer to hydrophilic chain extension, and then further acid water dispersion chain extension to form hydrophilic covalent bonding system of macromolecules and polymers step by step. At the same time, the multifunctional, high molecular and water-soluble self emulsification of silane coupling agent are realized.
The type, quantity and distribution of hydrophilic groups, carbon functional groups and silicon functional groups on the main and side chains of water-soluble polymer silane coupling agent can be designed according to the application requirements, in order to obtain a unique new environment-friendly functional material with excellent wetting and permeability for different substrate surfaces and curing at room temperature.
Wherein, n = 15 ~ 150, R1: epoxy hydrocarbon or triethoxysilyl hydrocarbon or alkane, R2: polyether 1 hydrocarbon or epoxy hydrocarbon or triethoxysilyl hydrocarbon or alkane, R3: alkane or polyether 1 hydrocarbon, R4: triethoxysilyl hydrocarbon or isocyanate hydrocarbon, R5: cyclooxyalkyl or trimethoxysilyl hydrocarbon, R6: polyether 2 hydrocarbon, R7: polyether 3 alkyl group or triethoxysilyl alkyl group, R8: polyether 4 alkyl group, R9: polyene polyamine alkyl group or isocyanate alkyl group, except that it can also be connected with sulfur-containing alkyl group, fluorine-containing alkyl group, etc. The bridging group - [bridge] - can be polymethylsiloxane, acrylic resin, polyurethane resin, epoxy resin, polyaminoic acid, etc.
In order to improve the service performance, the synthetic design of water-soluble polymer silane coupling agent should consider: (1) increase the variety and number of silicon functional groups and carbon functional groups as needed: the number of silicon functional groups of water-soluble polymer silane coupling agent can reach six, nine, twelve or even several, so the number of available precursors is huge. Coupling and crosslinking can further expand the precursor network at the same time, The amount and type of materials that can be hybridized are almost infinite. After the sol-gel reaction, the molecular characterization can be seen as bridged polysilsesquioxane with a bulk structure, and a number of carbon functional groups such as hydroxyl group, mercapto group, ammonia group, carboxyl group, alkene group, epoxy group, isocyanate group, and so on. The introduction of fluoroalkyl group can increase the application adaptability of silane coupling agent precursor network; (2) The - R arm connected between the functional group and the main chain is correspondingly extended to fully expose the functional group as far as possible to avoid shielding due to steric hindrance; (3) introducing the bridging structure similar to the substrate surface, side chain or macromolecule to improve the similarity between the water-soluble polymer silane coupling agent and the surface of the material substrate, making it easy to form a network like, bulk polysiloxane sol-gel with different characteristics of the substrate.
Because water-soluble polymer silane coupling agent can be flexibly designed into specific functional group combination according to specific application occasions, it can break through the limitation that the functional group of small molecule silane coupling agent is single and insoluble in water, and expand the silane coupling agent from the existing application field to the surface coupling hybrid modification of organic-inorganic, organic-biological-inorganic and other substrates Promote similar and compatible fields, especially where water is used as reaction medium, such as tanning, synthetic leather and textile finishing; Leather, fur and woolen products are washed, shrink proof and soft; Lubrication, rust prevention and anti-corrosion treatment of metal surfaces such as automobiles and machinery; Improve the adhesion and water resistance of water-based coatings and water-based waterproof inks; Organic surface modification and water resistance treatment of nano powder and hollow glass beads; Modification of stone plastic, wood plastic, plastic steel and other composite materials; Preparation of bio sol-gel hybrid materials; LED, medical human implant materials, biomedical engineering, etc
Invention content
1. Silane tanned leather
"Silane tanned leather" is a new word created by Chengdu Kate silicone new material technology Co., Ltd. In the professional field, the meaning of a new word is often not only a new combination of words, but also a new thing from new materials to new applications. Due to its good wettability, permeability, dispersion and compliance, silicone products have been favored by the leather industry as a development trend for more than 20 years. It may bring a progress and a change.
The introduction of silicone system into the process from raw leather to finished leather to solve the disadvantages of traditional leather making has entered the imagination of leather experts as early as last century. However, due to the large professional span, it is necessary to integrate the professional knowledge of polymer synthetic chemistry, water-soluble organic polymer bridged polysilsesquioxane precursor synthetic chemistry, leather chemical materials and leather technology, And there are no ready-made materials that can be operated, let alone reference use methods. From the perspective of the difficulty of implementation, it is tantamount to climbing the cloud.
Now, the development of the third generation silane modified leather chemical material system with silicon-based reaction activity and the related application system of the invention "silane tanned leather" produced by Chengdu Wenjiang Mingnida silicon fluoride leather application research and test factory has finally brought the scientific research idea of the older generation of experts from the laboratory to the market and landed smoothly. Silane tanning leather is a silane sol gel tanning technology which is characterized by quality improvement, cost reduction, water saving, energy saving and emission reduction. It is a non toxic, pollution-free water-soluble polymethylsiloxane bridged polysilsesquioxane precursor polymer silane coupling agent as the main framework. Tanning leather is regarded as the preparation of organic bio inorganic hybrid material in silane tanning system. According to the specific conditions of the market and raw material skin, the natural biopolymer skin collagen fiber is modified by inorganic, semi inorganic and organic sol-gel modification in different degrees to obtain expected performance. The invention advances the application of silicone materials in the field of leather making from the existing coating and fatliquoring section to the pre tanning preparation and tanning retanning section of water plant, filling the technical gap at home and abroad. On the basis of taking water-soluble polymer silane coupling agent as the main leather making material, the simple technical system of silane tanning for water saving, emission reduction, low carbon and environmental protection has been basically established, It has opened up a new road of water saving and emission reduction for traditional tanning for many years. Based on ecological leather cleaner production, it not only strives to pursue the environmental protection ecology of end products, but also always pays attention to the environmental protection ecology of product production process, controls pollution from the source of materials and processes, improves the situation of high energy consumption, high water consumption and high pollution in traditional tanning industry, and promotes the simplification, scientization and Artistry and promoting the development of tanning practice and modernization have a positive impact.
2. Selection of silane tanning agent
From a chemical point of view, the process of tanning is essentially the inorganic, semi inorganic and organic coupling hybrid modification of natural organic polymer skin collagen fibers with multi alkali coupling agents, such as inorganic, semi inorganic and organic multi alkali coupling agents Condensation cross-linking or addition cross-linking reaction of transition metal ion hydroxyl complexes with 4D or 5D empty orbits or their alkoxides (i.e. the - Oh is replaced by - or group) or organic compounds containing hydroxyl units (or hydroxyl units can be reduced in water) or other activated carbon functional groups with active hydrogen on skin collagen fibers.
Traditional tanned leather is mainly tanned with basic trivalent chromium. In acidic water environment, trivalent chromium is usually used as the central ion to form coordination compounds with three electron rich ligands in the form of d2sp3 hybrid. R-o-cr formed by dehydration and crosslinking with active hydrogen on skin collagen fibers can be regarded as a kind of polychromoxane. Due to the stable and hard structure of chromium, skin collagen fibers are endowed with good stability and rigidity after chromium modification. Theoretically, chromium ion can form octahedral coordination structure with six ligands at most. However, due to the mismatch between the electron orbital energy level and symmetry of chromium atom and carbon atom, it is difficult to form electron cloud flow between chromium and carbon, that is, it is difficult to form covalent bond, Therefore, after the coordination of hexavalent chromium ion (d2sp3) with three electron rich ligands, the remaining three empty coordination positions can not accept hydrocarbon groups, that is, Cr-C bond can not be formed. Therefore, chromium is not organic enough. It can better penetrate into skin collagen fibers only in the state of low pH aqueous solution, and the corresponding polychromoxane chrome tanned leather, i.e. blue wet leather, is not flexible enough, After the process, a large amount of grease must be filled to increase the flexibility and lubrication. If the leather blank is placed for a long time, the grease will be lost, which is easy to harden and age, affecting the quality. Although trivalent chromium is still the dominant material in the traditional tanning system, due to the toxicity of its hexavalent ions, it is harmful to the environment and human body. In addition, the earth's Chromium resources are becoming increasingly scarce, so the search for a more ideal alternative tanning agent has not stopped. Theoretically, any transition metal or semi metal element that can form three or more hydroxyl or alkoxy alkoxide coordination compounds, that is, transition metal or semi metal elements with 3D, 4D or 5D empty orbits, may have tanning function. It is better to be directly connected with carbon, i.e. - R. at the same time, it also requires good stability, hardness, softness, safety and non toxicity.
On the periodic table, the element that can be connected with three or more hydroxyl or alkoxy groups and can be directly connected with - R is silicon with 3D empty orbit. Nano sized inorganic silica can be used as a hydrogen bonded filler in leather making, but its activity is not enough to be used as tanning agent. In organosilicon, the silane coupling agent is r-si (or ') 3 structure, but the oil-soluble small molecular silane coupling agent on the market is insoluble in water, the - R is short, and the variety and number of functional groups are limited, so it is not suitable to be used as tanning agent. It is a bold idea to use the water-soluble polymer silane coupling agent with multiple active silicon functional groups and carbon functional groups in leather making. The synthesized water-soluble organic polymer bridged polysilsesquioxane precursor is specially used for leather making water field. At the same time, it has the characteristics of inorganic and organic tanning agents, non-toxic and pollution-free, and the earth is rich in silicon reserves, Therefore, it may be a suitable choice for tanning agent.
3. Comparison of silane tanning agent and chrome tanning agent
The Si atom radius on the silicon functional group Si (or ') 3 of silane coupling agent is large, the 3D orbit is empty and lacks electrons, while the 2p orbit of oxygen atom in - (or) 3 is electron rich. The orbital energy levels of the two are similar and symmetrical, and they are unified and opposite in the same molecule- (or) 3 can be delocalized and alcoholized into multi base structure - (OH) 3, which is similar to the coordination compound with three - Oh formed by trivalent chromium in acidic water environment. It can also cross-linked with active hydrogen dehydration (or dealcoholization) on skin collagen fibers. The water soluble polymer silane coupling agent has some silicon functional groups on the main and side chains, so it can react with the active hydrogen on the collagen fiber to form a network of polysiloxane sol-gel precursor structure. In the polysiloxane sol-gel system, the tanning cross linking of each layer of the leather is relatively homogeneous, which can better avoid the problem of loosening the surface of the chrome tanning which is caused by uneven tanning.
The tetravalent Si atom of water-soluble polymer silane coupling agent is SP3 hybrid, which is directly connected with the carbon atom to form si-r covalent bond. Therefore, the organic property is obviously better than trivalent chromium, and the similarity and compatibility with biological substrates such as skin collagen fiber are greatly increased. It does not need to be used strictly at low pH value like chrome tanning. At the same time, The macromolecular bridged-r group of water-soluble polymer silane coupling agent can be flexible according to needs, such as polysiloxane, polyurethane, polyacrylic acid resin, polypeptide, grease, etc. it is also endowed with different characteristics to play a role on different substrate surfaces and applications. Chrome tanning agents and other metal tanning agents such as zirconium, titanium and aluminum can not directly connect with carbon atoms to form M-R organic metal covalent bonds. The so-called organic chromium coupling agent, titanate coupling agent, alkoxy aluminum and other "metal organic compounds", their hydrocarbon groups are only indirectly connected with chromium, titanium and aluminum through oxygen. Therefore, in contrast, the reaction between silane and skin collagen fibers is easier, the molecular structure is more flexible, and it is easier to give different functions.
In addition, the water-soluble polymer silane coupling agent itself has unique stability and flexibility. Polysiloxane sol gel hybrid modified collagen fibers also have unique stability, flexibility, flexural and compressive resilience, silicone soft texture and other qualities, and the durability of these qualities. These properties are difficult for chrome alkane modified skin collagen fibers.
4. Comparison between silane tanning agent and organic tanning agent
The carbon atom of the organic tanning agent has (or can be reduced in water) active units that can react with the active hydrogen cross-linking on the surface of the substrate, such as dehydratable cross-linked hydroxyl Oh, dealcoholic cross-linked alkoxy or, adductable cross-linked isocyanate Group-N = C = O, etc. In the organic tanning agent molecule, the carbon atom with SP3 hybrid cannot be stably connected to three hydroxyl groups or alkoxy groups at the same time as the silicon atom on the silane coupling agent. The carbon atom with one - Oh is alcohol, the water loss with two - Oh is aldehyde, the water loss with three - oh is carboxylic acid, and the water loss with four - Oh can be regarded as "carbon dioxide". Therefore, hydroxyalkyl structure (phenolic resin of phenolic hydroxyl group, tetrahydroxymethylphosphine salt, cyanamide resin, etc.) and structure that can be reduced to single or multiple hydroxyl units in water, such as epoxy structure (epoxy resin), aldehyde structure (aldehyde tanning agent), carboxyl structure (acrylic resin tanning agent), oxazolidine structure (prepared by aldehyde synthesis and releasing aldehyde in water) Isocyanate structure (polyurethane resin tanning agent, which can be regarded as dialdehyde unit containing hydroxyl substituted by amino group) has certain tanning property.
The characteristic [Q-R '- Si (R) NX (3-N)] structure of water-soluble polymer silane coupling agent can contain multiple active silicon functional groups X and multiple different active carbon functional groups Q. In theory, the active carbon functional groups with organic tanning agents and the water-soluble polymer silane coupling agents can be used as the organic tanning agents. They can also act as organic tanning agents on the skin collagen fibers and form a sol-gel hybrid network with the silicon functional groups.
Because organic tanning agents can only rely on carbon functional groups, and the radius of carbon atoms on organic tanning agents is smaller than that of silicon atoms, cross-linking hybrids of skin collagen fibers are difficult to form homogeneous pore like network sol-gel, like polymer silane coupling agents with silicon functional groups and carbon functional groups. Therefore, the uniformity of tanned leather and the packaging ability of other leather materials must be inferior.
5. Role of silane tanning agent in tanning
To sum up, the main functions of water-soluble polymer silane coupling agents in tanning are: (1) through the cross linking of active silicon functional groups and carbon functional groups and collagen fibers, a sol-gel precursor network structure system of polysiloxane skin collagen fibers is constructed, and the unique and delicate soft and elastic silicone texture of leather is given. (2) Its excellent permeability, dispersion and special phase inversion properties play a unique role in regulating the penetration, absorption, emulsification and dispersion of various materials in the bath solution, such as acid, alkali, chrome tanning agent, grease, filler, dye and perfume, in skin collagen fiber. Therefore, the water-saving, emission reduction and environmental protection scheme without washing in the retanning and dyeing section can be realized; (3) the sol-gel precursor network of silane skin collagen fiber still has the precursor activity, and has the ability of cross-linking and binding to other materials such as tanning agents, dyestuffs, fats, fillers, spices and so on in the bath liquid, so that these materials can penetrate into the fiber together and are repackaged in a wide range of polysiloxane sol-gel network systems. Therefore, the leather quality can be maintained for a long time.
6. Technical route of silane tanning
In fact, water-soluble polymer silane coupling agent can be used throughout the whole leather manufacturing process, from water field to finishing, from fur to blank to finished products, as well as the upgrading and reuse of abnormal loose leather at all stages and the later washing care of leather and fur products.
In recent years, from a small number of water tanning tests to a pilot test to a small batch of leather processing, silane tanning leather has accumulated a lot of first-hand information. The technology of silane tanning and dyeing without washing has been mature. Using silane sol gel tanning method, alkali leather, nitrate or acid skin can be directly tanned from the wet blue section to completely change the tanning mode of low pH value chrome tanning, high pH value, high temperature fatliquoring and repeated water washing for more than 100 years. The user experience brought by silane tanned leather is unmatched by traditional carbon tanned leather in terms of leather quality, quality controllability, ease of operation, water saving, emission reduction, low carbon and environmental protection.
In addition, the silane tanning system is very inclusive. It can not only contain trivalent chromium, organic tanning agent and other traditional leather materials, but also contain other metal or mineral tanning agents such as zirconium, titanium, aluminum, iron and silicate. Even calcium, magnesium and zinc, which are not usually used as tanning agents, may be better integrated into the silane tanning system after silylation, Organic biological inorganic hybrid co modification was carried out on skin collagen fibers to make the hybrid modification more adjustable. On the other hand, all organic silane tanned leather without any metal tanning agent can also replace the cumbersome traditional oil tanning leather to obtain polysiloxane silicone rubber with soft and delicate, skin friendly and environmental protection, which can be used as underwear fabric. This silicone rubber fiber is cotton like and has memory function similar to memory alloy. Even if it shrinks and deforms at high temperature, once it returns to normal temperature, It will automatically restore the shape and feel before deformation. The wet and heat resistance, mechanical strength are better than traditional oil tanned leather, and the production cycle is short and the process is simple.
It can be seen that water-soluble, non-toxic and non polluting water-soluble polymer silane coupling agents are applied in leather making field. They are not only introduced into the traditional tannery process as a class of excellent additives, but also a kind of material that plays a leading role. They can be used to build a new water-saving, energy saving and emission reducing silane sol gel tanning technology system, according to the raw materials and market demand. It combines with other traditional tanning agents in varying degrees, so as to contain and screen carbon leather materials.
7. Silica gel tannin extract combined tanning scheme
In order to overcome the defects of traditional vegetable tanned leather, the invention provides a water-saving and emission reduction silane tanned leather manufacturing process of environmental friendly silica gel tannin extract combined tanning close to skin ecological flexible vegetable tanned leather, which can eliminate the hard, dead soft and poor hand feeling of vegetable tanned leather, improve the leather quality, simple process operation, save time by more than 50%, save water by more than 40%, and have a wide application range. In order to achieve the above purpose, the invention is realized by the following technical scheme:
The water-saving and emission reducing silane tanning process of environment-friendly silica gel tannin extract combined tanning, close to skin ecological flexible vegetable tanned leather includes silane soaking of fur, silica gel ash covering and wool pushing, silane alkali sulfide wool destroying and liming, silica gel re liming, silane hydrogen peroxide pre Liming (eliminating alkali sulfide), silane hydrogen peroxide main Liming (eliminating alkali sulfide), cationic silica gel pretreatment, salt leaching, acid leaching Silicone aldehyde primary tanning / silica gel tannin extract combined primary tanning, cationic silica gel softening, anionic silica gel tannin extract dyeing, retanning, filling and fatliquoring, cationic silica gel fixation and mildew proof treatment can save more than 50% of time, save more than 40% of water, and significantly reduce pollutant emissions and consumption of water, electricity and human resources.
In order to achieve the above purpose, the invention is realized through the following technical scheme: the water-soluble high molecular polyamine silane coupling agent completely replaces the water-saving and emission reduction silane tanning process of biological enzyme preparation, including fur silane soaking, silica gel coating and wool pushing, silane alkali sulfide wool destroying and soaking, silica gel re ashing, silane hydrogen peroxide pre deashing (eliminating alkali sulfide) Silane hydrogen peroxide main deashing (elimination of alkali sulfide), cationic silica gel pretreatment, salt leaching, acid leaching, silicone aldehyde primary tanning / silica gel tannin extract combination primary tanning, cationic silica gel softening, anionic silica gel tannin extract dyeing retanning filling fatliquoring, cationic silica gel fixation and mildew proof treatment.
The silane soaking step of the fur is as follows: weigh 100 parts of fur by weight in the drum, wash with water for 10 minutes, add 100-150 parts of normal temperature water, 0.1-1 parts of kt1717, 0.05-0.3 parts of kt3007, 0.2-0.5 parts of non-ionic degreasing agent, 0.1-0.3 parts of bactericide, 0.3-1 parts of soda ash and 0.1-0.3 parts of sodium sulfide, rotate slowly for 3 hours, rotate for 30 minutes / stop for 30 minutes, and rotate for 8-10 hours without soaking enzyme Degreasing enzyme, drum out, meat removal, silica gel bag ash and hair pushing;
The silica gel ash coating and roughening steps are as follows: 5000 parts of water, 30-60 parts of kt1717, 15-40 parts of kt3007, 20-40 parts of Liming additives, 30-60 parts of non-ionic degreasing agent, 60-100 parts of sodium hydrosulfide and 240-280 parts of sodium sulfide by weight; Mix well, then slowly add 3000-4000 parts of lime and stir while adding to obtain mortar. Apply the wrapped mortar on the rabbit skin and meat surface, appropriately increase the amount of application of the back ridge line, overlap the meat, stand for 6-12 hours, push the wool, drum in, and enter the silane alkali sulfide to destroy the wool and soak in ash;
The silane alkali sulfide wool destroying and liming steps are as follows: add 10-30 parts of normal temperature water, 0.1-0.3 parts of kt1717, 0.3-0.5 parts of non-ionic degreasing agent, 0.3-0.5 parts of Liming assistant, 0.5-0.8 parts of sodium hydrosulfide and 0.5-0.8 parts of sodium sulfide, turn for 30 minutes / stop for 30 minutes and 2 hours after slow rotation for 1 hour; Add 0.5-1 part of kt1717, 0.5-1.5 part of alkali sulfide and 1-3 part of lime, turn for 30 minutes / stop for 30 minutes and turn for 2 hours; Add 0.5-1 part of kt1717, 0.5-1.5 part of alkali sulfide and 1-3 part of lime, turn for 30 minutes / stop for 30 minutes and turn for 2-12 hours; Check the wool destruction. After the wool is destroyed, add 1-5 parts of kt1717, rotate for 2 hours, add 30-50 parts of normal temperature water, 1-2 parts of lime and 0.1-0.3 parts of Liming Agent, rotate for 30 minutes / stop for 30 minutes and stop for 2 hours; Add 50-150 phr of normal temperature water, 1-2 phr of lime and 0.1-0.3 phr of Liming aid, turn for 30 minutes / stop for 30 minutes, turn for 5 minutes / stop for 55 minutes after 2 hours, and turn for 10-24 hours. In this step, the drum skin is produced without Liming enzyme and other alkaline enzymes. The waste liquid is retained and can be recycled as Liming solution or re Liming solution, and then enter silica gel for re Liming;
The silica gel re ashing steps are as follows: weigh 100 parts of alkali skin into the drum by weight, add 100-200 parts of wool destroying Liming waste liquid, add 1-2 parts of kt1717, 0.3-0.5 parts of non-ionic degreasing agent and 3-5 parts of lime, turn slowly for 30 minutes / stop for 30 minutes and stop for 4-12 hours; In this step, no Liming enzyme or other alkaline enzymes are used. The waste liquid can be retained and recycled as Liming solution or re Liming solution. Wash the ash skin with water and enter silane hydrogen peroxide for pre deashing (eliminate alkali sulfide);
The silane hydrogen peroxide pre deashing (eliminating alkali sulfide) steps are as follows: adding 50-100 parts of normal temperature water, 2-4 parts of kt1717, 0.3-0.5 parts of non-ionic degreasing agent, and rotating slowly for 2 hours; Add 5-8 parts of ammonium sulfate and 0.5-1 part of deashing agent, and rotate slowly for 2 hours; Add 1-2 parts of hydrogen peroxide, rotate slowly for 4 hours, rotate slowly for 30 minutes / stop for 30 minutes, and stop for 4-12 hours; This step does not use softening enzymes such as trypsin and 1398 alkaline enzyme. After washing to pH 6.5-7.5, it enters cationic silica gel for pretreatment;
The pretreatment steps of cationic silica gel are as follows: add 30-50 parts of 35 ℃ hot water, 3-5 parts of kt1717 and 3-5 parts of kt4031, rotate slowly for 3 hours, and enter salt leaching;
The salt leaching step is: adding 8-10 parts of industrial salt and 8-10 parts of sodium sulfate, slowly rotating at 35 degrees for 3 hours, and entering acid leaching;
The acid leaching step is as follows: add 0.5-1.5 parts of industrial formic acid, adjust the pH value range to 2.5-3, rotate slowly for 8-12 hours, and enter silicone aldehyde primary tanning / silica gel tannin extract combined primary tanning;
The initial tanning steps of silicone aldehyde / silica gel tannin extract combination are as follows: adding 3-5 parts of kt2811, 0.1-0.3 parts of acid resistant oil and 2-4 parts of kt2034, and rotating slowly for 4-8 hours; Add 8-16 parts of tannin extract, 2-4 parts of acid resistant oil, 4-6 parts of kt2034 and 2-4 parts of kt5901, and rotate slowly for 8-12 hours; Add 1-2 parts of acid resistant oil and 2-4 parts of kt2034, adjust the temperature to 45 ℃, and rotate slowly for 8-12 hours; Leave the drum to stand for 48 hours, squeeze and cut evenly, and enter the cationic silica gel to soften;
The softening step of the cationic silica gel is as follows: weigh 100 parts of the peeled primary tanning skin according to the weight, put it in the drum, wash it twice, and adjust the temperature to 45 ℃; Add 100-150 parts of water at 45 ℃, kt4031 5-8 parts, kt1717 5-8 parts and kt2811 1-3 parts, rotate at medium speed for 4-6 hours, add 1-2 parts of baking soda and rotate at medium speed for 4-6 hours. This step does not need acid enzyme treatment, enter anionic silica gel tannin extract dyeing retanning, filling and fatliquoring;
The anionic silica gel tannin extract dyeing, retanning, filling and fatliquoring steps are as follows: adding x parts of dye, 3-5 parts of tannin extract, 2-4 parts of kt5901, 6-8 parts of kt2034, 4-6 parts of kt2351, 3-5 parts of acid resistant oil, 5-8 parts of general oil, rotating at a medium speed of 45 ℃ for 8-12 hours in the same bath, and entering cationic silica gel fixation and mildew prevention treatment;
The cationic silica gel fixing and anti mildew treatment steps are as follows: adding formic acid in the same bath to adjust the pH value to 3-3.5, rotating at a medium speed of 45 ℃ for 1 hour, adding 1-3 parts of kt4031, 0.3-0.5 parts of anti mildew agent, rotating at a medium speed of 45 ℃ for 2 hours, washing twice, bulging, drying and finishing to obtain leather blank.
Preferably, the KT1717 is a soft replacement and silane, and KT1717 is a side polyalkyl polyhydroxyalkyl triethoxy silyl based polymethyl silsesquioxane water emulsion with weak cationic emulsion polymerization. Also known as water-soluble organosilicon polymer silane coupling agent and low temperature coupling self crosslinking ammonium alkyl hydroxy silicone oil, the technical specifications are: 20 degree density 0.95 g/ml, water soluble matter content 20 + 1%. Solvent water, pH 6.5 ± 0.2, viscosity 40-50 MPa S, the appearance is light blue emulsion.
Preferably, kt3007 is an osmotic crosslinking silane assistant, kt3007 is an aqueous solution of multi epoxy alcohol ether alkyl polymethylsiloxane silane coupling agent isopropanol, and the technical indexes are: 20 ℃ density 0.85g/ml, weight percentage of nonvolatile components 36 ± 1%, solvent water, pH value 6.5 ± 0.2, charge non-ionic, viscosity 90-110mpa s. The appearance is light yellow to colorless transparent liquid.
Preferably, kt4031 is cationic polyurethane retanning silica gel, kt4031 is a water-soluble cationic polyurethane polymer silane coupling agent with coupling crosslinking activity, and it is also a strong cationic polyalkoxysiloxane carbamate grease silica gel polymer; The technical indexes are: 20 ℃ density 0.95 g / ml-1.05 g / ml, water soluble content 18-22%, solvent water, pH value 4.5 ± 0.3, viscosity 400-500 MPa s. The appearance is milky yellow emulsion.
Preferably, kt2811 is aminosilane modified fatty aldehyde, and kt2811 is a water-soluble silicone polyethylenepolyamine alkaline polymer silane coupling agent, which has good crosslinking, hybrid modification, penetration and dispersion. The technical specifications are: pH 2-4, weak cationic charge and appearance of light blue emulsion.
Preferably, the kt2034 is a cotton bubble meat feeling filled silica gel, and kt2034 is a secondary derivative of lecithin and hydroxyalkyl aminoalkyl carboxyalkyl polyalkoxysilalkyl modified polymethylsiloxane. The technical indexes are: 20 ℃ density 0.92 g / ml, water-soluble content 26-30%, solvent water, pH value 3.8 ± 0.2, viscosity 150-180mpa s. The appearance is light milky yellow thick liquid;
Preferably, kt5901 is a silicone sulfone filled synthetic tanning agent, kt5901 is a silicone sulfone bridged structure high-quality filling performance polymer tanning agent for secondary hydrolysis and condensation of naphthol sulfonic acid and SO2 organic derivatives, with technical indexes of 20 ℃, density: 1.10g/ml-1.25 g / ml, water-soluble content of 46% - 50%, solvent water, pH value: 4.0 ± 0.2, viscosity: 120MPa · s-140mpa · s, The appearance is light brown translucent thick liquid.
Preferably, kt2351 is a foamed elastic fatliquoring silicone oil, kt2351 is a modified polymeric silicone oil, and a water emulsion copolymer of modified reactive silicone oil and vinyl amino and carboxyl monomers. The technical indexes are: 20 ℃ density 1.10 g / ml-1.25 g / ml, water soluble content 28-33%, solvent water, pH value 4.5-5.5, viscosity 24000-26000 MPa s. The appearance is milky yellow thick liquid.
The invention relates to a silane tanning process of replacing enzyme preparation with water-soluble polyamine silane coupling agent, which has the advantages of simple and stable operation mode and easy to understand process. Save more than 50% of time and more than 40% of water, significantly reduce the emission of pollutants and the consumption of water, electricity, manpower and other resources.
In the traditional tanning process, biological enzyme preparation is repeatedly used in the process from fur to primary tanning and retanning, resulting in the quality defects of loose leather surface or the quality accidents of collagen digestion and scrapping caused by the uncontrollable or uncontrollable destruction of the natural cross-linking structure of collagen fibers, which brings serious psychological pressure to the operators of traditional tanning process. Water soluble polymer polyamine silane coupling agent replaces biological enzyme preparation for leather soaking, wool destruction, liming, re liming, deashing and other processes, and completely cancels the traditional enzyme softening process. As a cross-linking agent, it can effectively maintain or strengthen the cross-linking degree of natural cross-linking structure of skin collagen fibers. As a polyamine silane coupling agent, it can safely and effectively soften skin collagen fibers, Thus, the quality defects of loose leather surface or the quality accidents of leather collagen digestion and scrapping caused by the uncontrollable or uncontrollable destruction of the natural cross-linking structure of skin collagen fiber by biological enzyme preparation are eliminated, and the serious psychological pressure of leather loose surface and leather collagen digestion and scrapping quality accidents caused by biological enzyme preparation to the operators of traditional leather making process is effectively alleviated, The "good leather comes out of the silica gel ash tank", so that the process operators can easily control and obtain the soft but not loose high-quality silica gel fleshy leather quality.
Description of drawings
Fig. 1 is the structural diagram of water-soluble polymer silane coupling agent.
Fig. 2 is a technical roadmap for the application of water-soluble polymer silane coupling agent in the field of leather making.
Specific embodiments
The invention will be further described in detail below in combination with specific embodiments.
Example 1: using the water-soluble high molecular polyamine silane coupling agent of the invention to completely replace the water-saving and emission reduction silane tanning process of biological enzyme preparation to produce environment-friendly silica gel tannin extract combined tanning close to skin ecological flexible buffalo skin vegetable tanning mat leather, including fur silane soaking, silane sulfurization alkali hair destruction liming, silica gel liming, silane hydrogen peroxide pre Liming (eliminating alkali sulfide) Silane hydrogen peroxide main deashing (elimination of alkali sulfide), cationic silica gel pretreatment, salt leaching, acid leaching, silicone aldehyde primary tanning / silica gel tannin extract combined primary tanning, cationic silica gel softening, anionic silica gel tannin extract dyeing retanning filling fatliquoring, cationic silica gel fixation and mildew proof treatment. The specific steps are as follows:
(1) Silane soaking of fur: weigh 100 parts of buffalo fur by weight and put it in the drum, wash it with water for 10 minutes, add 150 parts of normal temperature water, 0.5 parts of kt1717, 0.1 parts of kt3007, 0.3 parts of non-ionic degreasing agent, 0.1 parts of bactericide, 0.5 parts of soda ash and 0.3 parts of sodium sulfide, turn it slowly for 3 hours, turn it for 30 minutes / stop for 30 minutes, and stop it for 10 hours. In this step, do not use soaking enzyme and degreasing enzyme, take out the drum, remove the meat and trim the edge, Entering silane alkali sulfide for wool destruction and liming;
(2) Silane alkali sulfide wool destroying Liming: Add 20 parts of normal temperature water, 0.3 parts of kt1717, 0.3 parts of non-ionic degreasing agent, 0.5 parts of Liming assistant, 0.6 parts of sodium hydrosulfide and 0.6 parts of sodium sulfide. After slow rotation for 1 hour, turn for 30 minutes / stop for 30 minutes and turn for 2 hours; Add 0.5 parts of kt1717, 0.6 parts of alkali sulfide and 2 parts of lime, turn for 30 minutes / stop for 30 minutes and turn for 2 hours; Add 0.5 parts of kt1717, 0.6 parts of alkali sulfide and 2 parts of lime, turn for 30 minutes / stop for 30 minutes and turn for 10 hours; Check the wool destruction. After the wool is destroyed, add 3 parts of kt1717, rotate for 2 hours, add 30 parts of normal temperature water, 1 part of lime and 0.2 parts of Liming Agent, rotate for 30 minutes / stop for 30 minutes and stop for 2 hours; Then add 80 parts of normal temperature water, 2 parts of lime and 0.3 parts of Liming aid, turn for 30 minutes / stop for 30 minutes, turn for 5 minutes / stop for 55 minutes after stopping for 2 hours, and turn for 24 hours. In this step, liming enzyme is not used, drum skin is produced, and the waste liquid is retained, which can be recycled as Liming solution or re Liming solution, and then enter silica gel for re Liming;
(3) Silica gel re ashing: weigh 100 parts of alkali skin into the drum, add 200 parts of wool destroying Liming waste liquid, add 1 part of kt1717, 0.5 parts of non-ionic degreasing agent and 3 parts of lime, turn slowly for 30 minutes / stop for 30 minutes and stop for 10 hours; No Liming enzyme is needed in this step. The waste liquid can be retained and recycled as Liming solution or re Liming solution. Wash the ash skin with water and enter silane hydrogen peroxide for pre deashing (eliminate alkali sulfide);
(4) Silane hydrogen peroxide pre deashing (eliminating alkali sulfide): add 50 parts of normal temperature water, 1 part of kt1717 and 0.3 parts of non-ionic degreasing agent, and rotate slowly for 2 hours; Add 3 parts of ammonium sulfate and 0.5 parts of deashing agent and rotate slowly for 2 hours; Add 1 part of hydrogen peroxide and rotate slowly for 4 hours. In this step, do not use softening enzymes such as trypsin and 1398 alkaline enzyme, wash with water, and enter silane hydrogen peroxide for main deashing (eliminate alkali sulfide);
(5) Silane hydrogen peroxide main deashing (eliminating alkali sulfide): add 30 parts of normal temperature water, 2 parts of kt1717 and 0.3 parts of non-ionic degreasing agent, and rotate slowly for 2 hours; Add 8 parts of ammonium sulfate and 0.5 parts of deashing agent and rotate slowly for 2 hours; Add 1 part of hydrogen peroxide, turn slowly for 4 hours, turn slowly for 30 minutes / stop for 30 minutes, and turn and stop for 10 hours; In this step, softening enzymes such as trypsin and 1398 alkaline enzyme are not used. After washing to pH 6.5-7.5, it enters cationic silica gel for pretreatment;
(6) Pretreatment of cationic silica gel: add 30 parts of 35 ℃ hot water, 3 parts of kt1717 and 3 parts of kt4031, rotate slowly for 3 hours, and enter salt leaching;
(7) Salt leaching: add 8 parts of industrial salt and 8 parts of sodium sulfate, rotate slowly at 35 ℃ for 3 hours, and enter acid leaching;
(8) Pickling: add 1.5 phr of industrial formic acid, adjust the pH value range to 2.5-3, rotate slowly for 8 hours, and enter the silicone aldehyde primary tanning / silica gel tannin extract combined primary tanning
(9) Silicone aldehyde primary tanning / silica gel tannin extract combined primary tanning: add 4 parts of kt2811, 0.3 parts of acid resistant oil and 4 parts of kt2034, and rotate slowly for 6 hours; Add 12 parts of tannin extract, 4 parts of acid resistant oil, 6 parts of kt2034 and 3 parts of kt5901, and rotate slowly at 35 ℃ for 10 hours; Add 2 parts of acid resistant oil and 4 parts of kt2034, adjust the temperature to 45 ℃, and rotate slowly for 10 hours; Leave the drum to stand for 48 hours, squeeze and cut evenly, and enter the cationic silica gel to soften;
(10) Cationic silica gel softening: weigh 100 parts of the well shaved primary tanned leather in the drum, wash twice, and adjust the temperature to 45 ℃; Add 100 parts of water at 45 ℃, 6 parts of kt4031, 6 parts of kt1717 and 2 parts of kt2811, rotate at medium speed for 4 hours, add 2 parts of baking soda and rotate at medium speed for 4 hours. This step does not need acid enzyme treatment, and enter anionic silica gel tannin extract dyeing retanning and filling fatliquoring;
(11) Anionic silica gel tannin extract dyeing retanning filling fatliquoring: add x parts of dye, 5 parts of tannin extract, 2 parts of kt5901, 5 parts of kt2034, 5 parts of kt2351, 3 parts of acid resistant oil and 8 parts of fatliquoring agent in the same bath, rotate at a medium speed of 45 ℃ for 6 hours, and enter cationic silica gel for fixation and mildew proof treatment;
(12) Cationic silica gel fixation and anti mildew treatment: add formic acid in the same bath to adjust the pH value to 3-3.5, rotate at a medium speed of 45 ℃ for 1 hour, add 2 parts of kt4031 and 0.3 parts of anti mildew agent, rotate at a medium speed of 45 ℃ for 2 hours, wash twice, drum out, and enter the drying process to obtain the skin blank.
The above industrial products such as kt1717, kt3007, kt2811, kt4031, kt2034, kt5901 and kt2351 are purchased from Chengdu Wenjiang Mingnida silicon fluoroleather application research and test factory. The environment-friendly silica gel tannin extract combined with tanning, close to the skin, ecological and flexible buffalo skin vegetable tanning mat produced by the invention is cool but not ice, mild and delicate when in close contact with human skin, that is, cool and comfortable without cold stimulation and discomfort, with the fine and smooth feeling of real silk without the roughness and stiffness of cotton and hemp.
Example 2: using the water-soluble high molecular polyamine silane coupling agent of the invention to completely replace the water-saving and emission reduction silane tanning process of biological enzyme preparation to produce environment-friendly silica gel tannin extract combined tanning close to the skin and ecological flexible smooth rabbit skin bra inner skin friendly leather, including fur silane soaking, silica gel ash covering and wool pushing, silane alkali sulfide wool destroying and liming Silane hydrogen peroxide pre deashing (eliminating alkali sulfide), silane hydrogen peroxide main deashing (eliminating alkali sulfide), cationic silica gel pretreatment, salt leaching, acid leaching, silaldehyde primary tanning / silica gel tannin extract combined primary tanning, cationic silica gel softening, anionic silica gel tannin extract dyeing retanning filling fatliquoring, cationic silica gel fixation and mildew proof treatment. The specific steps are as follows:
(1) Silane soaking of fur: weigh 100 parts of rabbit fur by weight and put it in the drum, wash it with water for 10 minutes, add 150 parts of normal temperature water, 0.5 parts of kt1717, 0.1 parts of kt3007, 0.3 parts of non-ionic degreasing agent, 0.1 parts of bactericide, 0.5 parts of soda ash and 0.3 parts of sodium sulfide, rotate slowly for 3 hours, rotate for 30 minutes / stop for 30 minutes, and stop for 10 hours. In this step, do not soak enzyme and degreasing enzyme, take out the drum, and cut off the head and tail Limbs, drain and moisturize, and push hair into silica gel.
(2) Silica gel coating and roughening: 5000 parts of water, 40 parts of kt1717, 20 parts of kt3007, 20 parts of Liming additives, 50 parts of non-ionic degreasing agent, 80 parts of sodium hydrosulfide and 250 parts of sodium sulfide by weight; Mix well, then slowly add 3000 parts of lime and stir while adding to obtain mortar. Coat the coated mortar on the rabbit skin and meat surface, appropriately increase the application amount of the back line, overlap the meat, stand and stack for 6-12 hours, push the wool, enter the drum, enter the silane alkali sulfide to destroy the wool and immerse in ash.
(3) Silane alkali sulfide wool destroying Liming: Add 20 parts of normal temperature water, 0.3 parts of kt1717, 0.3 parts of non-ionic degreasing agent, 0.5 parts of Liming assistant, 0.6 parts of sodium hydrosulfide and 0.6 parts of sodium sulfide. After slow rotation for 1 hour, turn for 30 minutes / stop for 30 minutes and turn for 4 hours; Check the wool destruction. After the wool is destroyed, add 3 parts of kt1717, rotate for 2 hours, add 30 parts of normal temperature water, 1 part of lime and 0.2 parts of Liming Agent, rotate for 30 minutes / stop for 30 minutes and stop for 2 hours; Add 80 phr of normal temperature water, 2 phr of lime and 0.3 phr of Liming aid, turn for 30 minutes / stop for 30 minutes, turn for 5 minutes / stop for 55 minutes after 2 hours, and turn for 24 hours. In this step, liming enzyme is not needed. The waste liquid can be retained and recycled as Liming solution or re Liming solution, and then enter silane dioxygen water for pre Liming (eliminating alkali sulfide).
(4) Silane hydrogen peroxide pre deashing (eliminating alkali sulfide): add 50 parts of normal temperature water, 1 part of kt1717 and 0.3 parts of non-ionic degreasing agent, and rotate slowly for 2 hours; Add 3 parts of ammonium sulfate and 0.5 parts of deashing agent and rotate slowly for 2 hours; Add 1 part of hydrogen peroxide and rotate slowly for 4 hours. In this step, do not use softening enzymes such as trypsin and 1398 alkaline enzyme, wash with water, and enter silane hydrogen peroxide for main deashing (eliminate alkali sulfide).
(5) Silane hydrogen peroxide main deashing (eliminating alkali sulfide): add 30 parts of normal temperature water, 2 parts of kt1717 and 0.3 parts of non-ionic degreasing agent, and rotate slowly for 2 hours; Add 8 parts of ammonium sulfate and 0.5 parts of deashing agent and rotate slowly for 2 hours; Add 1 part of hydrogen peroxide, turn slowly for 4 hours, turn slowly for 30 minutes / stop for 30 minutes, and turn and stop for 10 hours; In this step, softening enzymes such as trypsin and 1398 alkaline enzyme are not used. After washing to pH 6.5-7.5, it enters cationic silica gel for pretreatment.
(6) Pretreatment of cationic silica gel: add 30 parts of 35 ℃ hot water, 3 parts of kt1717 and 3 parts of kt4031, rotate slowly for 3 hours, and enter salt leaching.
(7) Salt leaching: add 8 parts of industrial salt and 8 parts of sodium sulfate, rotate slowly at 35 ℃ for 3 hours, and enter the acid leaching.
(8) Pickling: add 1.5 phr of industrial formic acid, adjust the pH value range to 2.5-3, rotate slowly for 8 hours, and enter silicone aldehyde primary tanning / silica gel tannin extract combined primary tanning.
(9) Silicone aldehyde primary tanning / silica gel tannin extract combined primary tanning: add 4 parts of kt2811, 0.3 parts of acid resistant oil and 4 parts of kt2034, and rotate slowly for 6 hours; Add 12 parts of tannin extract, 4 parts of acid resistant oil, 6 parts of kt2034 and 3 parts of kt5901, and rotate slowly at 35 ℃ for 10 hours; Add 2 parts of acid resistant oil and 4 parts of kt2034, adjust the temperature to 45 ℃, and rotate slowly for 10 hours; Leave the drum to stand for 48 hours, squeeze and cut evenly, and enter the cationic silica gel to soften.
(10) Cationic silica gel softening: weigh 100 parts of the well shaved primary tanned leather in the drum, wash twice, and adjust the temperature to 45 ℃; Add 100 parts of water at 45 ℃, 6 parts of kt4031, 6 parts of kt1717 and 2 parts of kt2811, rotate at medium speed for 4 hours. This step does not need acid enzyme treatment, add 2 parts of baking soda, rotate at medium speed for 4 hours, enter anionic silica gel tannin extract dyeing Retanning, filling and fatliquoring.
(11) Anionic silica gel tannin extract dyeing retanning filling fatliquoring: add x parts of dye, 5 parts of tannin extract, 2 parts of kt5901, 5 parts of kt2034, 5 parts of kt2351, 3 parts of acid resistant oil and 8 parts of fatliquoring agent in the same bath, rotate at a medium speed of 45 ℃ for 6 hours, and enter cationic silica gel for fixation and mildew proof treatment.
(12) Cationic silica gel fixation and anti mildew treatment: add formic acid in the same bath to adjust the pH value to 3-3.5, rotate at a medium speed of 45 ℃ for 1 hour, add 2 parts of kt4031 and 0.3 parts of anti mildew agent, rotate at a medium speed of 45 ℃ for 2 hours, wash twice, drum out, and enter the drying process to obtain the skin blank.
The above industrial products such as kt1717, kt3007, kt2811, kt4031, kt2034, kt5901 and kt2351 are purchased from Chengdu Wenjiang Mingnida silicon fluoroleather application research and test factory. The environment-friendly silica gel tannin extract combined with tanning, close to the skin, ecological and flexible smooth rabbit skin bra inner skin friendly leather produced by the invention, when in close contact with breast nipples, is soft and delicate, moisture and breathable, free and transparent, mildew and sterilization proof, has good skin physiological respiratory function, has fine and smooth silk without rough and stiff cotton and hemp.
Example 3: using the water-soluble high molecular polyamine silane coupling agent of the invention to completely replace the water-saving and emission reduction silane tanning process of biological enzyme preparation to produce environment-friendly silica gel tannin extract combined tanning, close to skin ecological flexible sheep leather chest outer supporting lining leather, including fur silane immersion, silica gel coated wool pushing, silane alkali sulfide wool destruction liming, silica gel re liming Silane hydrogen peroxide pre deashing (eliminating alkali sulfide), silane hydrogen peroxide main deashing (eliminating alkali sulfide), cationic silica gel pretreatment, salt leaching, acid leaching, silaldehyde primary tanning / silica gel tannin extract combined primary tanning, cationic silica gel softening, anionic silica gel tannin extract dyeing retanning filling fatliquoring, cationic silica gel fixation and mildew proof treatment. The specific steps are as follows:
(1) Silane soaking of fur: weigh 100 parts of cotton wool skin by weight and put it into the drum, wash it with water for 10 minutes, add 150 parts of normal temperature water, 0.5 parts of kt1717, 0.1 parts of kt3007, 0.3 parts of non-ionic degreasing agent, 0.1 parts of bactericide, 0.5 parts of soda ash and 0.3 parts of sodium sulfide, rotate slowly for 3 hours, rotate for 30 minutes / stop for 30 minutes, and rotate for 10 hours. In this step, do not use soaking enzyme and degreasing enzyme, take out the drum, cut off the head, tail Limbs, drain and moisturize, and push hair into silica gel.
(2) Silica gel coating and roughening: the formula of coating mortar is: 5000 parts by weight, 40 parts by kt1717, 20 parts by kt3007, 20 parts by liming additives, 50 parts by non-ionic degreasing agent, 80 parts by sodium hydrosulfide and 250 parts by sodium sulfide; Mix well, then slowly add 3000 parts of lime and stir while adding to obtain mortar. Coat the coated mortar on the surface of sheep skin and meat, increase the amount of dorsal ridge line, overlap the meat, stand for 12-24 hours, push the wool, drum, and enter silane alkali sulfide to destroy the wool and soak in ash.
(3) Silane alkali sulfide wool destroying Liming: Add 20 parts of normal temperature water, 0.3 parts of kt1717, 0.3 parts of non-ionic degreasing agent, 0.5 parts of Liming assistant, 0.6 parts of sodium hydrosulfide and 0.6 parts of sodium sulfide. After slow rotation for 1 hour, turn for 30 minutes / stop for 30 minutes and turn for 4 hours; Check the wool destruction. After the wool is destroyed, add 3 parts of kt1717, rotate for 2 hours, add 30 parts of normal temperature water, 1 part of lime and 0.2 parts of Liming Agent, rotate for 30 minutes / stop for 30 minutes and stop for 2 hours; Add 80 phr of normal temperature water, 2 phr of lime and 0.3 phr of Liming aid, turn for 30 minutes / stop for 30 minutes, turn for 5 minutes / stop for 55 minutes after 2 hours, and turn for 24 hours. This step does not need Liming enzyme. The waste liquid can be retained and recycled as Liming solution or re Liming solution, and then enter silica gel for re Liming.
(4) Silica gel re ashing: add 200 parts of wool destroying Liming waste liquid, 1 part of kt1717, 0.5 parts of non-ionic degreasing agent and 3 parts of lime. Turn slowly for 30 minutes / stop for 30 minutes and stop for 10 hours. Liming enzyme is not needed in this step. The waste liquid can be retained and recycled as Liming solution or re ashing solution. Wash the ash skin dry and enter silane hydrogen peroxide for pre deashing (eliminate alkali sulfide).
(5) Silane hydrogen peroxide pre deashing (eliminating alkali sulfide): add 50 parts of normal temperature water, 1 part of kt1717 and 0.3 parts of non-ionic degreasing agent, and rotate slowly for 2 hours; Add 3 parts of ammonium sulfate and 0.5 parts of deashing agent and rotate slowly for 2 hours; Add 1 part of hydrogen peroxide and rotate slowly for 4 hours. In this step, do not use softening enzymes such as trypsin and 1398 alkaline enzyme, wash with water, and enter silane hydrogen peroxide for main deashing (eliminate alkali sulfide).
(6) Silane hydrogen peroxide main deashing (eliminating alkali sulfide): add 30 parts of normal temperature water, 2 parts of kt1717 and 0.3 parts of non-ionic degreasing agent, and rotate slowly for 2 hours; Add 8 parts of ammonium sulfate and 0.5 parts of deashing agent and rotate slowly for 2 hours; Add 1 part of hydrogen peroxide, turn slowly for 4 hours, turn slowly for 30 minutes / stop for 30 minutes, and turn and stop for 10 hours; In this step, softening enzymes such as trypsin and 1398 alkaline enzyme are not used. After washing to pH 6.5-7.5, it enters cationic silica gel for pretreatment.
(7) Pretreatment of cationic silica gel: add 30 parts of 35 ℃ hot water, 3 parts of kt1717 and 3 parts of kt4031, rotate slowly for 3 hours, and enter salt leaching.
(8) Salt leaching: add 8 parts of industrial salt and 8 parts of sodium sulfate, rotate slowly at 35 ℃ for 3 hours, and enter acid leaching.
(9) Pickling: add 1.5 parts of industrial formic acid, adjust the pH value range to 2.5-3, rotate slowly for 8 hours, and enter the initial tanning of silicone aldehyde / silica gel tannin extract.
(10) Silicone aldehyde primary tanning / silica gel tannin extract combined primary tanning: add 4 parts of kt2811, 0.3 parts of acid resistant oil and 4 parts of kt2034, and rotate slowly for 6 hours; Add 12 parts of tannin extract, 4 parts of acid resistant oil, 6 parts of kt2034 and 3 parts of kt5901, and rotate slowly at 35 ℃ for 10 hours; Add 2 parts of acid resistant oil and 4 parts of kt2034, adjust the temperature to 45 ℃, and rotate slowly for 10 hours; Leave the drum to stand for 48 hours, squeeze and cut evenly, and enter the cationic silica gel to soften.
(11) Cationic silica gel softening: weigh 100 parts of the well shaved primary tanned leather in the drum, wash twice, and adjust the temperature to 45 ℃; Add 100 parts of water at 45 ℃, 6 parts of kt4031, 6 parts of kt1717 and 2 parts of kt2811, rotate at medium speed for 4 hours, add 2 parts of baking soda and rotate at medium speed for 4 hours. This step does not need acid enzyme treatment, and enter anionic silica gel tannin extract dyeing retanning and filling fatliquoring.
(12) Anionic silica gel tannin extract dyeing retanning filling fatliquoring: add x parts of dye, 5 parts of tannin extract, 2 parts of kt5901, 5 parts of kt2034, 5 parts of kt2351, 3 parts of acid resistant oil and 8 parts of fatliquoring agent in the same bath, rotate at a medium speed of 45 ℃ for 6 hours, and enter cationic silica gel for fixation and mildew proof treatment.
(13) Cationic silica gel fixation and anti mildew treatment: add formic acid in the same bath to adjust the pH value to 3-3.5, rotate at a medium speed of 45 ℃ for 1 hour, add 2 parts of kt4031 and 0.3 parts of anti mildew agent, rotate at a medium speed of 45 ℃ for 2 hours, wash twice, drum out, and enter the drying process to obtain the skin blank.
The above industrial products such as kt1717, kt3007, kt2811, kt4031, kt2034, kt5901 and kt2351 are purchased from Chengdu Wenjiang Mingnida silicon fluoroleather application research and test factory. The environment-friendly silica gel tannin extract combined with tanning, close to the skin, ecological and flexible smooth sheepskin leather chest outer supporting lining leather produced by the invention has soft texture, elasticity, crisp and easy to set, fine hand feeling and free and transparent; Especially in the inner layer of the bra, the sandwich between the skin and rabbit's outer skin can be placed in the design of the special breast health care package, which has special nursing effect for dredging the breast meridians, preventing breast hyperplasia and breast cancer. At the same time, it has the breast tissue to lift up and make the breast full and sexy. It can avoid the harmful and harmful breast damage caused by traditional toxic and harmful sponge, plastic foam and other breast filling materials. In addition, it can absorb sweat, not easy to deform, easy to take care of and store, self-cleaning, etc. it has more powerful functions than similar materials.
The technical scheme provided by the embodiment of the invention is introduced in detail above. In this paper, specific examples are applied to elaborate the principle and implementation mode of the embodiment of the invention. The description of the above embodiment is only applicable to help understand the principle of the embodiment of the invention; Meanwhile, for those skilled in the art, according to the embodiment of the invention, there will be changes in the specific implementation mode and application scope. In conclusion, the contents of the specification should not be understood as restrictions on the invention.